Au NCs were synthesized according to the traditional seed-mediated method In a typicalstep Au seeds were first synthesized by adding 06 ml of 001 M NaBH4 in a mixturesolution of 01 ml of 25 mM HAuCl4
Au纳米晶体的合成采用传统的种子介导法。在典型的步骤中,首先制备Au种子,将0.6毫升0.01M NaBH4加入到25 mM HAuCl4和0.1 M CTAB的混合溶液中。将上述溶液放置在30摄氏度的水浴中,不搅动。1小时后,将种子溶液通过将1毫升种子溶液加入到9毫升Milli-Q水中进行稀释。然后,将5微升稀释后的种子溶液加入到生长溶液中,生长溶液包含1.6毫升0.1 M CTAB,0.2毫升7 mM HAuCl4,8毫升Milli-Q水和1.2毫升0.1 M AA。上述溶液在30摄氏度的水浴中不搅动过夜。最终产物通过7830 rpm的离心10分钟收集,并最终重新分散到Milli-Q水中以供进一步使用。